Virtual Process Laboratory

← monprocess.org · Course home

Virtual Lab · GMIT Raw Material Process Engineering

Virtual Process Laboratory

Four laboratory benches that behave like the real ones: you choose the conditions, run the test, take the readings, and every measurement carries realistic experimental scatter. The data go into your lab notebook, and you evaluate them the same way you would in the GMIT mineral processing and hydrometallurgy laboratories: linearisations, kinetic fits, Arrhenius plots, energy balances.

01 · PrepareRead the objective and answer the pre-lab check.
02 · RunSet the conditions and run the bench. Repeat runs to build a series.
03 · RecordEvery run is logged in the notebook below each bench. Export it as CSV.
04 · EvaluateFit the model to your own data. The evaluation questions are checked against your runs.
Bench 1 · Rod/ball mill + √2 sieve stack

Grinding and sieve analysis: P80 and Bond energy

Grind a 500 g sample of −2 mm ore in the laboratory ball mill, screen it through a √2 sieve series and build the cumulative-passing curve. From the curve you determine the product P80 and, with the Bond work index, the specific grinding energy W = 10·Wi·(1/√P80 − 1/√F80).

Conditions INPUT

Feed F80 = 2000 µm. Sample mass 500.0 g. Wet-screen at 38 µm before dry sieving. A mass loss above 1 % invalidates the test.

Pre-lab check PREP

Why is a √2 sieve series used?

Cumulative passing vs size (log axis). Dashed line: 80 % passing.
Rosin–Rammler linearisation: ln(−ln(1−F)) vs ln x. The slope is the uniformity index n.

Evaluation REPORT

1 · Read the P80 of your last run from the curve (log-linear interpolation between sieves), in µm.

2 · Calculate the Bond specific energy for your last run, in kWh/t.

3 · Determine the Rosin–Rammler uniformity index n from the linearisation (slope).

Bench 2 · 2.5 L Denver-type cell

Batch flotation kinetics of a copper sulphide ore

Float 1000 g of a 0.62 % Cu chalcopyrite ore and collect five timed concentrates. You fit the first-order model R = R∞(1 − e^(−kt)) to the cumulative recovery and study how collector dosage, pH, air rate and grind size act on R∞, on k and on the grade–recovery curve.

Conditions INPUT

Concentrates are scraped every 10 s and pooled into C1 (0–1 min), C2 (1–2), C3 (2–4), C4 (4–8) and C5 (8–15 min). Frother MIBC 20 g/t, conditioning 3 min.

Pre-lab check PREP

Why does the pH stay above 10 in copper rougher flotation?

Cumulative Cu recovery vs time: measured points and the fitted first-order model.
Grade–recovery curve: all logged runs, one colour per run.

Evaluation REPORT

1 · Fit the first-order model to your last run. What is the rate constant k, in min⁻¹?

2 · What is the ultimate recovery R∞, in %?

3 · Calculate the combined grade of C1 + C2 (% Cu) from the masses and assays.

Bench 3 · 1 L jacketed glass reactor

Leaching kinetics of an oxide copper ore in sulphuric acid

Leach 50 g of a 2.0 % Cu oxide ore in 0.5 L H₂SO₄ and sample the solution over two hours. You test the three shrinking-core models (film diffusion, chemical reaction, product-layer diffusion), identify the rate-controlling step, and obtain the activation energy from runs at several temperatures.

Conditions INPUT

Samples of 5 mL are taken at 5, 10, 20, 30, 45, 60, 90 and 120 min, filtered and analysed for Cu by AAS; X is corrected for the copper removed with the samples. Fit the models to points with X < 0.95 only.

Pre-lab check PREP

Which observation points most clearly to chemical-reaction control?

Copper extraction X vs time for all logged runs.
Shrinking-core linearisations g(X) vs t for the last run, with R² of each model.
Arrhenius plot ln k vs 1000/T from runs at equal acid, size and stirring.

Evaluation REPORT

1 · Which model gives the best linear fit for your last run? (1 = film diffusion, 2 = chemical reaction, 3 = product-layer diffusion)

2 · Rate constant k of the chemical-reaction model for your last run, 1−(1−X)^(1/3) = k·t, in min⁻¹ (e.g. 0.0042).

3 · Activation energy from your Arrhenius plot, in kJ/mol (at least three temperatures, other conditions equal).

Bench 4 · Laboratory EW cell, Pb–Ca–Sn anode

Copper electrowinning: current efficiency and energy

Plate copper onto a 10 × 10 cm stainless-steel blank from a synthetic advance electrolyte. You weigh the cathode, calculate the current efficiency from Faraday’s law, break the cell voltage down into its components and work out the specific energy in kWh per tonne of copper.

Conditions INPUT

Cathode area 0.0100 m² (one face, edges masked). Anode–cathode gap 40 mm. H₂SO₄ 180 g/L, guar 250 g/t Cu. Balance readability 0.01 g.

Pre-lab check PREP

Which side reaction lowers the current efficiency most in copper EW?

Cell voltage breakdown for the last run: E_rev, anode and cathode overpotential, electrolyte IR drop, contacts.
Current efficiency and specific energy against current density for all logged runs.

Evaluation REPORT

1 · Theoretical copper mass for your last run (Faraday, M = 63.55 g/mol, z = 2), in g.

2 · Current efficiency from the weighed mass, in %.

3 · Specific energy consumption, in kWh per tonne Cu.

Lab notebook

Every run on every bench is stored in this browser. Export the notebook as CSV for your report, or clear it to start a new series.

Pilot-plant stations

To plan and record the real tests in the GMIT laboratory, use ProLab, the laboratory experiment planner. Once the bench data are understood, scale up: the full-circuit simulators run the same unit operations at plant scale, with operator HMIs, control loops and fault injection.

Models behind the benches

Bench 1: product size distribution after Rosin–Rammler, F(x) = 1 − exp[−(x/x′)ⁿ]; P80 falls with grinding time according to a first-order breakage approximation scaled by the Bond work index; per-sieve masses carry ±0.4 % weighing scatter and a 0.2–0.8 g handling loss. Bench 2: first-order flotation of the copper mineral, R∞ and k depending on collector coverage, pH (pyrite depression above pH 10), particle size (fine and coarse losses) and air rate; gangue is recovered by entrainment with the water. Bench 3: shrinking-core model with resistances in series, t = τ_f·X + τ_r·[1 − (1−X)^⅓] + τ_d·[1 − 3(1−X)^⅔ + 2(1−X)]; E_a = 48 kJ/mol for the surface reaction and 12 kJ/mol for diffusion; the film term falls with stirring speed. Bench 4: Faraday’s law with parasitic Fe³⁺ reduction and a mass-transfer penalty near the limiting current; Tafel overpotentials, IR drop from the electrolyte conductivity, E_rev = 0.89 V.

Virtual Process Laboratory · Dr. Togtokhbaatar Purev-Ochir, GMIT Faculty of Raw Materials and Environmental Engineering · Data are generated by teaching models calibrated to typical laboratory values; they are not plant data.